GOST 5017-2006
GOST 5017−2006 Bronze tin pressure treated. Brand
GOST 5017−2006
Group W51
INTERSTATE STANDARD
BRONZE TIN PRESSURE TREATED
Brand
Wrought tin bronzes. Grades
ISS 77.120.30
GST 17 3620
17 3630
Date of introduction 2008−01−01
Preface
Goals, basic principles and main procedure of works on interstate standardization have been established in GOST 1.0−92 «interstate standardization system. Basic provisions» and GOST 1.2−97* «interstate standardization system. Interstate standards, rules and recommendations on interstate standardization. The procedure of development, adoption, application, renewal and cancellation"
_______________
* On the territory of the Russian Federation the document is not valid. Valid GOST 1.2−2009. — Note the manufacturer’s database.
Data on standard
1 DEVELOPED by the Technical Committee for standardization TC 106 «Tsvetmetprokat», Scientific-research, project and design Institute for alloys and processing of nonferrous metals «joint-stock company «Institute tsvetmetobrabotka» (JSC «Institute tsvetmetobrabotka»)
2 SUBMITTED by the Technical Secretariat of the Interstate Council for standardization, Metrology and certification
3 ACCEPTED by the Interstate Council for standardization, Metrology and certification (Protocol No. 29 of June 24, 2006)
The standard was accepted by voting:
Short name of the country by MK (ISO 3166) 004−97 |
Country code by MK (ISO 3166) 004−97 |
Abbreviated name of the national authority for standardization |
Azerbaijan |
AZ |
Azstandart |
Armenia |
AM |
The Ministry of trade and economic development of the Republic of Armenia |
Belarus |
BY |
Gosstandart Of The Republic Of Belarus |
Georgia |
GE |
Gosstandart |
Kazakhstan |
KZ |
Gosstandart Of The Republic Of Kazakhstan |
Kyrgyzstan | KG | Kyrgyzstandard |
Moldova |
MD |
Moldova-Standard |
Russian Federation |
EN |
Federal Agency on technical regulation and Metrology |
Tajikistan |
TJ |
Tajikstandart |
Turkmenistan |
TM |
The MDCSU «Turkmenstandartlary" |
Uzbekistan |
UZ |
Uzstandard |
Ukraine |
UA |
Derzhspozhyvstandart Of Ukraine |
4 by Order of the Federal Agency for technical regulation and Metrology dated December 27, 2006 No. 497-St inter-state standard GOST 5017−2006 introduced as a national standard of the Russian Federation from January 1, 2008
5 REPLACE GOST 5017−74
6 REISSUE. January 2008
Information about introduction in action (termination) of this standard is published in the index «National standards».
Information about the amendments to this standard is published in the index «National standards», and the text changes — in the information sign «National standards». In case of revision or cancellation of this standard the appropriate information will be published in the information index «National standards»
1 Scope
This standard applies to the tin bronze, pressure treated, intended for the manufacture of semi-finished products used in various industries.
When referring to the tin bronzes should indicate the brand in accordance with this standard.
2 Normative references
This standard uses the regulatory references to the following international standards:
GOST 1953.1−79 Bronze tin. Methods for determination of copper
GOST 1953.2−79 Bronze tin. Methods for determination of lead
GOST 1953.3−79 Bronze tin. Methods for determination of tin
GOST 1953.4−79 Bronze tin. Methods for determination of phosphorus
GOST 1953.5−79 Bronze tin. Methods for determination of Nickel
GOST 1953.6−79 Bronze tin. Methods for determination of zinc
GOST 1953.7−79 Bronze tin. Methods of iron determination
GOST 1953.8−79 Bronze tin. Methods for determination of aluminium
GOST 1953.9−79 Bronze tin. Methods for determination of silicon
GOST 1953.10−79 Bronze tin. Methods for determination of antimony
GOST 1953.11−79 Bronze tin. Methods for determination of bismuth
GOST 1953.12−79 Bronze tin. Methods of determining sulphur
GOST 1953.13−79 Bronze tin. Method of determination of manganese
GOST 1953.14−79 Bronze tin. Method for determination of magnesium
GOST 1953.15−79 Bronze tin. Methods for determination of arsenic
GOST 1953.16−79 Bronze tin. Method of determining titanium
GOST 30608−98 of Bronze tin. XRF technology
ST SEV 543−77 Number. Record rules and rounding
Note — When using this standard appropriate to test the effect of reference standards for the sign «National standards» drawn up as of January 1 of the current year and related information signs, published in the current year. If the reference document is replaced (modified), then the use of this standard should be guided by the replaced (modified) document. If the reference document is cancelled without replacement, then the situation in which the given link applies to the extent that does not affect this link.
3 Stamps
3.1 Brand, chemical composition and sample designation tin bronzes shall be as given in table 1.
Table 1 — Chemical composition of the tin bronzes
Mark |
Pre- Affairs |
Mass fraction, % |
Approximate appointment | |||||||||||
Item |
||||||||||||||
Cu copper |
Al aluminium tions |
Bi vis- Mut |
Fe same- the Uragan |
Ni no- Kel |
R Foz Fort |
Pb Swee- Heff |
Sb sur- mA |
Si cream tions |
Sn tin |
Zn zinc |
The amount of other elements tov |
|||
Brof8−0,3 |
Min. |
OST. |
- |
- |
- |
- |
0,26 |
- |
- |
- |
7,5 |
- |
- |
The wire used in the pulp and paper industry for the manufacture of meshes |
Max. |
- |
0,002 |
0,002 |
0,02 |
0,2 |
0,35 |
0,02 |
0,002 |
0,002 |
8,5 |
0,3 |
0,1 |
||
Brof7−0,2 |
Min. |
OST. |
- |
- |
- |
- |
0,10 |
- |
- |
- |
7,0 |
- |
- |
Bars, used in various industries |
Max. |
- |
0,002 |
0,002 |
0,05 |
0,2 |
0,25 |
0,02 |
0,002 |
0,005 |
8,0 |
0,3 |
0,1 |
||
Brof6,5−0,4 |
Min. |
OST. |
- |
- |
- |
- |
0,26 |
- |
- |
- |
6,0 |
- |
- |
The wire used in the pulp and paper industry for the manufacture of meshes and for springs, parts, tapes and bands used in mechanical engineering |
Max. |
- |
0,002 |
0,002 |
0,02 |
0,2 |
0,40 |
0,02 |
0,002 |
0,005 |
7,0 |
0,3 |
0,1 |
||
Brof6,5−0,15 |
Min. |
OST. |
- |
- |
- |
- |
0,10 |
- |
- |
- |
6,0 |
- |
- |
Tapes, strips, rods, used in mechanical engineering; bearing parts of the pipe-blank for the manufacture of bimetal bushings salebrosum |
Max. |
- |
0,002 |
0,002 |
0,05 |
0,2 |
0,25 |
0,02 |
0,002 |
0,002 |
7,0 |
0,3 |
0,1 |
||
Brof4−0,25 |
Min. |
OST. |
- |
- |
- |
- |
0,2 |
- |
- |
- |
3,5 |
- |
- |
Tube used in vehicle building and instrumentation |
Max. |
- |
0,002 |
0,002 |
0,02 |
0,2 |
0,3 |
0,02 |
0,002 |
0,002 |
4,0 |
0,3 |
0,1 |
||
Brof2−0,25 |
Min. |
OST. |
- |
- |
- |
- |
0,02 |
- |
- |
- |
1,0 |
- |
- |
Screws, tape for flexible hoses, conductive parts, filler material for welding |
Max. |
- |
- |
- |
0,05 |
0,2 |
0,30 |
0,03 |
- |
- |
2,5 |
0,3 |
0,3 |
||
Broc4−3 |
Min. |
OST. |
- |
- |
- |
- |
- |
- |
- |
- |
3,5 |
2,7 |
- |
Tapes, strips, rods, used in electrical engineering, mechanical engineering; wire springs and equipment chemical industry |
Max. |
- |
0,002 |
0,002 |
0,05 |
0,3 |
0,03 |
0,02 |
0,002 |
0,005 |
4,0 |
3,3 |
0,2 |
||
Brocs4−4-2,5 |
Min. |
OST. |
- |
- |
- |
- |
- |
1,5 |
- |
- |
3,0 |
3,0 |
- |
Tape used for gaskets, bushings and bearings |
Max. |
- |
0,002 |
0,002 |
0,05 |
0,3 |
0,03 |
3,5 |
0,002 |
- |
5,0 |
5,0 |
0,2 |
||
Brocs4−4-4 |
Min. |
OST. |
- |
- |
- |
- |
- |
3,5 |
- |
- |
3,0 |
3,0 |
- |
Tape used for gaskets, bushings and bearings |
Max. |
- |
0,002 |
0,002 |
0,05 |
0,3 |
0,03 |
4,5 |
0,002 |
- |
5,0 |
5,0 |
0,2 |
||
Notes 1 In bronze brand Brof6,5−0,15 allowed mass fraction of tin to 7.5%. 2 In bronze brand Broc4−3 allowed mass fraction of titanium is not more than 0.12% by mass fraction of copper, which is not included in the total amount of other elements. 3 In the alloys used for the manufacture of products with magnetic properties allowed mass fraction of iron no more than 0.02%. The symbol marks added to the letter A. 4 Mass fraction of sulphur and magnesium are allowed no more than 0.007% each. 5 the «— «Sign affixed simultaneously to the upper and lower limits of the mass fraction of the element indicates that this element is not specified and is determined only by the demand of the consumer and in this case, the content of the impurities included in the total amount of other elements. 6 Admixture should be considered as the element from which specified only a maximum limit to its content. 7 Impurities that are not listed in this table are considered in total other elements. |
3.2 Chemical composition of tin bronze depending on the grades determined according to GOST 1953.1−1953.16 GOST, GOST 30608.
Allowed the use of other methods of analysis, accuracy is not inferior to the above.
Arbitration methods of analysis point in the standards for specific types of products.
3.3 the analysis Results of each element are rounded according to the rounding rules established ST SEV 543, with the precision provided by table 1.
In disputable cases the results of the analysis is determined with the accuracy specified in the arbitration method of measurements.