By visiting this site, you accept the use of cookies. More about our cookie policy.

Steel 25KHGT

Description

Steel 25KHGT

Steel 25KHGT: a brand of steels and alloys. Below is the systematized information on the purpose, chemical composition, types of supplies, substitutes, temperature of critical points, physical, mechanical, technological and casting properties for the grade — Steel 25HGT.

General information about steel 25HGT

Substitute brand
Steel: 18HGT, 30HGT, 25HGM.
Delivery type
Long products, including shaped: GOST 4543−71, GOST 259071, GOST 2591−71, GOST 2879−69. Calibrated bar GOST 7417−75, GOST 8559−75, GOST 8560−78, GOST 1051−73. Polished bar and silver bar GOST 14955−77. Strip GOST 103−76. Forgings and forged billets GOST 1133−71.
Application
Loaded gears and other parts, the hardness of which is more than HRCэ59.

Chemical composition of steel 25HGT

Chemical element %
Silicon (Si) 0.17−0.37
Manganese (Mn) 0.80−1.10
Copper (Cu), no more 0.30
Nickel (Ni), no more 0.30
Sulfur (S), no more 0.035
Titanium (Ti) 0.03−0.09
Carbon (C) 0.22−0.29
Phosphorus (P), no more 0.035
Chromium (Cr) 1.00−1.30

Mechanical properties of steel 25HGT

Heat treatment, delivery condition σ 0.2, MPa σ B, MPa δ 5 ,% ψ,% KCU, J / m 2
Bar. Normalization 880−950 ° C, air. Hardening 850 ° С, oil. Vacation 200 ° C, water, oil or air. 980 1270 ten 50 69
Cementation 920−950 ° С, air. Hardening 840−860 ° С, oil. Vacation 190−210 ° С, air. 1100 1500 nine   60

Technological properties of steel 25HGT

Forging temperature
Beginning 1220, end 800.
Weldability
RDS, KTS, subsequent heat treatment is required.
Tendency to release ability
inclined
Flock sensitivity
sensitive