Steel 15ps
Description
Steel 15ps
Steel 15ps: brand of steels and alloys. Below is a systematized information on the purpose, chemical composition, types of supplies, substitutes, temperature of critical points, physical, mechanical, technological and casting properties for the grade — Steel 15ps.
General information of steel 15ps
Substitute brand |
steel: 10kp, 20kp |
Delivery type |
Long products, including shaped: GOST 2590−71, GOST 2591−71, GOST 2879−69, GOST 19771−74, GOST 8278−83, GOST 10772−74, GOST 8281−80, GOST 8282−83, GOST 18283 -77, GOST 10702−78. Calibrated bar GOST 7417−75, GOST 8559−75, GOST 8560−78, GOST 10702−78. Polished rod and silverware GOST 14955−77. Thick sheet GOST 19903−74, GOST 4041−71, GOST 1577−81. Thin sheet GOST 19903−74, GOST 16523−70, GOST 19904−74. Tape GOST 10234−77, GOST 1530−78. Strip GOST 82−70, GOST 103−76, GOST 1577−81. Wire GOST 17305−71, GOST 2771−81, GOST 5663−79. Pipes GOST 10704−91, GOST 10705−80. |
Application |
Elements of pipe connections, fittings, plugs and other details of boiler and turbine construction, operating at temperatures from -40 to 425 ° С; after carburizing and cyanidation — parts that require high surface hardness and low core strength (fasteners, axles, levers, etc. parts). |
Chemical composition of steel 15ps
Chemical element |
% |
Silicon (Si) |
0.05−0.17 |
Manganese (Mn) |
0.35−0.65 |
Copper (Cu), no more |
0.25 |
Arsenic (As), no more |
0.08 |
Nickel (Ni), no more |
0.25 |
Sulfur (S), no more |
0.04 |
Carbon (C) |
0.12−0.19 |
Phosphorus (P), no more |
0.035 |
Chromium (Cr), no more |
0.25 |
Mechanical properties of steel 15ps
Mechanical properties of rolled products
Heat treatment, delivery condition |
σ B, MPa |
δ 5 ,% |
δ 4 ,% |
ψ,% |
HB |
Calibrated and calibrated steel with special finishing after annealing or tempering |
365−470 |
|
|
55 |
149 |
Steel calibrated and calibrated with a special finish, work-hardened without heat treatment |
390 |
8 |
|
50 |
187 |
Normalized and hot rolled sheets |
345 |
thirty |
|
|
|
Normalized or hot rolled strips |
355 |
29 |
|
55 |
|
Hot rolled sheets |
315−440 |
|
23 |
|
|
Cold rolled sheets |
315−440 |
|
|
|
|
Heat-treated sheets of the 1st-2nd category |
325−440 |
thirty |
|
|
121 |
Technological properties of steel 15ps
Forging temperature |
Beginning 1300, end 700. Air cooling. |
Weldability |
Can be welded without restrictions. Welding methods: RDS, ADS submerged arc and gas shielded, KTS. |
Machinability by cutting |
In the hot-rolled state at HB 143 K υ tv.spl. = 1.8. |
Tendency to release ability |
Not sensitive. |
Flock sensitivity |
Not inclined. |
Temperature of critical points of steel 15ps
Critical point |
° C |
Ac1 |
735 |
Ac3 |
863 |
Ar3 |
840 |
Ar1 |
685 |
Impact strength of steel 15ps
Impact strength, KCU, J / cm 2
Delivery status, heat treatment |
+20 |
-20 |
-thirty |
-40 |
-50 |
After normalization |
274 |
108 |
59 |
34 |
20 |
Physical properties of steel 15ps
Test temperature, ° С |
20 |
100 |
200 |
300 |
400 |
500 |
600 |
700 |
800 |
900 |
Normal elastic modulus, E, GPa |
201 |
192 |
185 |
172 |
156 |
|
|
|
|
|
Torsional shear elastic modulus G, GPa |
83 |
80 |
77 |
74 |
71 |
68 |
63 |
|
|
|
Density of steel, pn, kg / m 3 |
7850 |
7827 |
7794 |
7759 |
7724 |
7687 |
7648 |
7611 |
7599 |
7584 |
Thermal conductivity coefficient W / (m ° С) |
|
53 |
53 |
49 |
46 |
43 |
39 |
36 |
32 |
thirty |
Ud. electrical resistance (p, Nom. m) |
|
233 |
296 |
387 |
487 |
607 |
753 |
904 |
1092 |
1140 |
Test temperature, ° С |
20−100 |
20−200 |
20−300 |
20−400 |
20−500 |
20−600 |
20−700 |
20−800 |
20−900 |
20−1000 |
Linear expansion coefficient (a, 10−6 1 / ° С) |
12.4 |
13.2 |
13.9 |
14.5 |
14.9 |
15.1 |
15.3 |
|
|
|
Specific heat (C, J / (kg ° C)) |
465 |
486 |
515 |
532 |
565 |
586 |
620 |
691 |
708 |
|