Steel 10kp
Designation
Name |
The value |
Designation GOST Cyrillic |
10кп |
Designation GOST Latin |
10kp |
Transliteration |
10kp |
The chemical elements |
10 |
Description
10kp steel is used: for the manufacture of sheet metal, 1−2 mm 4−14 category, intended for cold forming; sheet rolled double-sided electrolytic coating and single-side polymer coating, used in the construction industry, commercial engineering, industrial ventilation, household appliances, decoration and other purposes; parts, operating at temperatures up to +450 °C, which are requirements of high plasticity; bushings, lugs, washers, screws and other parts after HTO (chemical heat treatment), requirements of high surface hardness and wear resistance at low strength core; welded pipes; enamelware; cold strip 0,05−4,00 mm, designed for bending, punching parts, manufacture of pipes, cored wire, parts, bearings and other metal products.
Note
The degree of deoxidation — KP.
Standards
Name |
Code |
Standards |
Sectional and shaped rolling |
В32 |
GOST 1050-88, GOST 7417-75, GOST 8560-78, GOST 10702-78, GOST 14955-77, GOST 1050-2013, TU 14-1-2118-77, TU 14-11-245-88, TU 14-1-1271-75, TU 14-136-367-2008 |
Sheets and stripes |
В33 |
GOST 1577-93, GOST 4041-71, GOST 13345-85, GOST 24244-80, TU 14-1-450-72, TU 14-1-4516-88 |
Classification, nomenclature and general norms |
В70 |
GOST 2771-81 |
Pipes steel and connecting parts to them |
В62 |
GOST 3262-75, GOST 10704-91, GOST 10705-80, GOST 10707-80, TU 14-3-1428-86, TU 14-3Р-63-2002, TU 1373-022-05757850-08, TU 1373-013-02949352-2003 |
Tapes |
В24 |
GOST 3560-73 |
Steel wire medium- and high-carbon |
В72 |
GOST 3920-70, GOST 7372-79, GOST 9389-75, GOST 9850-72, GOST 17305-91, GOST 26366-84 |
Tapes |
В34 |
GOST 503-81, GOST 10234-77, GOST 19851-74 |
Low-carbon steel wire |
В71 |
GOST 5663-79 |
Sheets and stripes |
В23 |
GOST 82-70, GOST 14918-80, GOST 16523-97, GOST 19904-90, GOST 16523-89, GOST 16523-70, GOST 19903-90, TU 14-1-4695-89 |
Sectional and shaped rolling |
В22 |
GOST 8278-83, GOST 8281-80, GOST 8282-83, GOST 8283-93, GOST 8319.0-75, GOST 9234-74, GOST 10551-75, GOST 11474-76, GOST 19771-93, GOST 19772-93, GOST 2590-2006, GOST 2879-2006 |
Bulls. Blanks. Slabs |
В31 |
OST 3-1686-90, TU 14-1-4944-90 |
Mechanical characteristics
Section, mm |
sT|s0,2, MPa |
σB, MPa |
d5, % |
d4 |
d |
d10 |
y, % |
Brinell hardness number, MPa |
HRB |
Tape flatted average strength of 0.1-4.0 mm according to GOST 10234-77 in the state of delivery (indicated delivery) |
- |
- |
490-780 |
- |
- |
- |
- |
- |
- |
- |
- |
- |
390-540 |
- |
- |
- |
- |
- |
- |
- |
- |
- |
540-690 |
- |
- |
- |
- |
- |
- |
- |
- |
- |
690-830 |
- |
- |
- |
- |
- |
- |
- |
- |
- |
≤440 |
- |
- |
≥20 |
- |
- |
- |
- |
- |
- |
≤410 |
- |
- |
- |
- |
- |
- |
- |
Cold-rolled steel strip 0,05-4,00 mm according to GOST 503-81 on delivery |
- |
- |
≥540 |
- |
- |
- |
- |
- |
- |
- |
≤1.5 |
- |
310-440 |
- |
≥17 |
- |
- |
- |
- |
- |
1.55-2 |
- |
310-440 |
- |
≥18 |
- |
- |
- |
- |
- |
2.1-2.9 |
- |
310-440 |
- |
≥20 |
- |
- |
- |
- |
- |
3-4 |
- |
310-440 |
≥24 |
- |
- |
- |
- |
- |
- |
2.1-2.9 |
- |
440-590 |
- |
≥4 |
- |
- |
- |
- |
- |
3-4 |
- |
440-590 |
≥4 |
- |
- |
- |
- |
- |
- |
≤1.5 |
- |
270-390 |
- |
≥23 |
- |
- |
- |
- |
- |
1.55-2 |
- |
270-390 |
- |
≥26 |
- |
- |
- |
- |
- |
2.1-2.9 |
- |
270-390 |
- |
≥30 |
- |
- |
- |
- |
- |
3-4 |
- |
270-390 |
≥32 |
- |
- |
- |
- |
- |
- |
≤1.5 |
- |
370-510 |
- |
≥7 |
- |
- |
- |
- |
- |
1.55-2 |
- |
370-510 |
- |
≥9 |
- |
- |
- |
- |
- |
2.1-2.9 |
- |
370-510 |
- |
≥10 |
- |
- |
- |
- |
- |
3-4 |
- |
370-510 |
≥12 |
- |
- |
- |
- |
- |
- |
Rolled sheet 1-2 categories of heat-treated (annealing, normalization, high tempering or normalizing + tempering) in the delivery state according to GOST 4041-71 |
4-14 |
- |
270-410 |
≥32 |
- |
- |
≥28 |
- |
≤114 |
≤64 |
Wire for cold heading as supplied by GOST 5663-79 |
- |
- |
440-590 |
- |
- |
- |
- |
≥55 |
- |
- |
- |
- |
≤590 |
- |
- |
- |
- |
≥55 |
- |
- |
Longitudinal electric-welded pipes (Dy=10-530 mm) in the delivery condition. Listed marsvolta base metal |
- |
≥196 |
≥314 |
≥25 |
- |
- |
- |
- |
- |
- |
Hot-rolled steel and hot rolled with special surface finish |
- |
- |
- |
- |
- |
- |
- |
- |
≤137 |
- |
- |
- |
- |
- |
- |
- |
- |
- |
≤115 |
- |
Steel calibrated and calibrated with special surface finish |
- |
- |
≥370 |
≥8 |
- |
- |
- |
≥55 |
≤179 |
- |
- |
- |
310-410 |
- |
- |
- |
- |
≥50 |
≤143 |
- |
- |
- |
290-390 |
- |
- |
- |
- |
≥50 |
≤143 |
- |
Hot-rolled sheet in the delivery condition. Group strength К270В |
≤2 |
- |
270-410 |
- |
≥24 |
- |
- |
- |
- |
≤65 |
2-3.9 |
- |
270-410 |
- |
≥26 |
- |
- |
- |
- |
≤65 |
Cold-rolled sheet in the delivery condition. Group strength К270В |
≤2 |
- |
270-410 |
- |
≥25 |
- |
- |
- |
- |
≤65 |
2-3.9 |
- |
270-410 |
- |
≥28 |
- |
- |
- |
- |
≤65 |
Cold roll for the enamelware according to GOST 24244-80 in the state of delivery (specify a group to exhaust the category of the quality) |
0.5-1.5 |
≥250 |
270-368 |
- |
≥30 |
- |
≥36 |
- |
- |
- |
1.5-2 |
≥235 |
270-368 |
- |
≥30 |
- |
≥36 |
- |
- |
- |
2-2.5 |
≥235 |
270-368 |
- |
≥32 |
- |
≥36 |
- |
- |
- |
0.5-2 |
- |
255-362 |
- |
≥28 |
- |
≥34 |
- |
- |
- |
2-2.5 |
- |
255-362 |
- |
≥30 |
- |
≥34 |
- |
- |
- |
0.5-2 |
- |
265-382 |
- |
≥26 |
- |
- |
- |
- |
- |
2-2.5 |
- |
265-382 |
- |
≥29 |
- |
- |
- |
- |
- |
0.5-2 |
- |
265-382 |
- |
≥25 |
- |
- |
- |
- |
- |
2-2.5 |
- |
265-382 |
- |
≥28 |
- |
- |
- |
- |
- |
Steel grooved on delivery |
≤25 |
- |
≥372 |
≥8 |
- |
- |
- |
≥55 |
- |
- |
Leaves heat-treated 1 and 2nd categories |
- |
- |
275-410 |
≥32 |
- |
- |
- |
- |
≤114 |
- |
Tape |
- |
- |
315-440 |
- |
≥17 |
- |
- |
- |
- |
- |
- |
- |
440-590 |
- |
≥4 |
- |
- |
- |
- |
- |
- |
- |
375-510 |
- |
≥7 |
- |
- |
- |
- |
- |
Description mechanical marks
Name |
Description |
Section |
Section |
sT|s0,2 |
Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2% |
σB |
Limit short-term strength |
d5 |
Elongation after rupture |
d4 |
Elongation after rupture |
d |
Elongation after rupture |
d10 |
Elongation after rupture |
y |
The relative narrowing |
HRB |
Rockwell hardness (indenter steel, spherical) |
Technological properties
Name |
The value |
Weldability |
Without limitation, except HTO parts; welding methods: SMAW, submerged arc ADS and gateway protection of the CCC. |
Propensity to temper brittleness |
Tend not. |
Forging temperature |
Beginning - 1300 °C, end - 700 °C. air Cooling. |
Flock-sensitive sensitivity |
not sensitive. |
Workability by cutting |
In hot rolled state at 99-107 blower SB and HB=450 MPa Kn TV.SPL.=Of 2.1 Kn b.St.=1,6. |