Steel A35
Designation
Name |
The value |
Designation GOST Cyrillic |
А35 |
Designation GOST Latin |
A35 |
Transliteration |
A35 |
The chemical elements |
- |
Description
A35 steel is used: for the production of complex-shaped parts, processed by CNC-machines and parts, which are increased requirements to the surface quality, operating at higher voltages and pressures (axles, rollers, bushings, rings, gears, fingers, screws, bolts, nuts).
Note
Sulfur carbon steel high machinability.
Standards
Name |
Code |
Standards |
Sectional and shaped rolling |
В52 |
GOST 13616-97, GOST 13617-97, GOST 13618-97, GOST 13619-97, GOST 13620-90, GOST 13621-90, GOST 13622-91, GOST 13623-90, GOST 13624-90, GOST 13737-90, GOST 13738-91, GOST 17575-90, GOST 17576-97, GOST 29296-92, GOST 29303-92, GOST Р 50066-92, GOST Р 50067-92, GOST Р 50077-92 |
Sectional and shaped rolling |
В32 |
GOST 1414-75, GOST 14955-77 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Cr |
Si |
Ni |
Fe |
Cu |
GOST 1414-75 |
0.32-0.4 |
0.08-0.15 |
≤0.06 |
0.7-1 |
≤0.25 |
0.15-0.35 |
≤0.25 |
The rest |
≤0.25 |
Fe is the basis.
Mechanical characteristics
Section, mm |
σB, MPa |
d5, % |
y, % |
Brinell hardness number, MPa |
The hot rolled, without heat treatment |
|
≥510 |
≥15 |
≥23 |
≤201 |
Rental of calibrated and full hard without heat treatment |
|
≥570 |
≥6 |
- |
≤229 |
Description mechanical marks
Name |
Description |
Section |
Section |
σB |
Limit short-term strength |
d5 |
Elongation after rupture |
y |
The relative narrowing |
Technological properties
Name |
The value |
Propensity to temper brittleness |
tend not |
Flock-sensitive sensitivity |
not sensitive |