Steel St3kp (ВСт3кп)
Designation
Name | The value |
---|---|
Designation GOST Cyrillic | Ст3кп |
Designation GOST Latin | Ct3kp |
Transliteration | St3kp |
The chemical elements | 3 |
Name | The value |
---|---|
Designation GOST Cyrillic | ВСт3кп |
Designation GOST Latin | BCt3kp |
Transliteration | VSt3kp |
The chemical elements | 3 |
Description
St3kp steel is used: for the manufacture of expanded metal sheets, lightly loaded elements and nesvorny welded structures and components operating at temperatures from -40 °C to +400 °C; the profiles used in the railcar industry; forgings seniam to 300 mm. strength classes KP 175, KP 195; hot pan and C-shaped profiles for agricultural machinery; corrugated steel rhombic and point for shipbuilding; profile housing final drive of the tractor; welded pipes for the manufacture of parts and structures in motovelotehnika; hot-rolled steel sheets with one-sided rhombic and lenticular corrugated; two-headed rails, t-type P5, is designed for ground and suspended tracks; steel bent closed welded square and rectangular sections, intended for use in agricultural machinery, tractor and other sectors of the economy; crutches accuracy class, designed for fastening of rails to wooden sleepers and bars.
Note
The degree of deoxidation — KP.
Standards
Name | Code | Standards |
---|---|---|
Tapes | В34 | GOST 19851-74 |
Pipes steel and connecting parts to them | В62 | GOST 3262-75, GOST 8696-74, GOST 10704-91, GOST 10705-80, GOST 10706-76, GOST 10707-80, GOST 12132-66, TU 14-3-1160-83, TU 14-3-1428-86, TU 14-3Р-56-2001, TU 1373-013-02949352-2003 |
Tapes | В24 | GOST 3560-73, GOST 6009-74, STP М309-74 |
Classification, nomenclature and general norms | В20 | GOST 380-2005 |
Sectional and shaped rolling | В22 | GOST 5267.0-90, GOST 5422-73, GOST 5781-82, GOST 7511-73, GOST 8239-89, GOST 8240-97, GOST 8278-83, GOST 8281-80, GOST 8282-83, GOST 8283-93, GOST 8509-93, GOST 8510-86, GOST 9234-74, GOST 10551-75, GOST 11474-76, GOST 12492.1-90, GOST 12492.13-90, GOST 12492.14-90, GOST 19240-73, GOST 19425-74, GOST 19771-93, GOST 19772-93, GOST 25577-83, GOST 30565-98, GOST 535-2005, GOST 30136-95, GOST 2590-2006, GOST 2591-2006, GOST 2879-2006, OST 5.9086-85, OST 5.9087-84, TU 14-2-341-78, TU 14-2-949-91, TU 14-1-5283-94, TU 14-1-5254-94 |
Rails. Lining. Lining. Crutches | В42 | GOST 5812-82, GOST 8142-89, GOST 16277-93 |
Sheets and stripes | В23 | GOST 82-70, GOST 8568-77, GOST 14637-89, GOST 14918-80, GOST 16523-97, GOST 19903-74, GOST 16523-89, GOST 16523-70, GOST 103-2006, GOST 19903-90, OST 5.9094-85, TU 36.26.11-5-89, TU 14-1-3023-80, STP М324-90 |
Metal forming. Forgings | В03 | GOST 8479-70, OST 5Р.9125-84, ST ЦКБА 010-2004 |
Bulls. Blanks. Slabs | В31 | OST 3-1686-90, TU 14-1-4944-90 |
Welding and cutting of metals. Soldering, riveting | В05 | OST 36-58-81 |
Sheets and stripes | В33 | TU 14-1-3579-83, TU 14-1-4431-88 |
Sectional and shaped rolling | В32 | TU 14-11-245-88, TU 14-1-1271-75, TU 14-136-367-2008 |
Mechanical characteristics
Section, mm | sT|s0,2, MPa | σB, MPa | d5, % | d4 | y, % | kJ/m2, кДж/м2 | Brinell hardness number, MPa |
---|---|---|---|---|---|---|---|
Longitudinal electric-welded pipes (Dy=10-530 mm) in the delivery condition. Listed marsvolta base metal | |||||||
- | ≥225 | ≥372 | ≥22 | - | - | - | - |
Forgings. Normalization | |||||||
100-300 | ≥175 | ≥355 | ≥24 | - | ≥50 | ≥590 | 101-143 |
100 | ≥175 | ≥355 | ≥28 | - | ≥55 | ≥640 | 101-143 |
100-300 | ≥195 | ≥390 | ≥23 | - | ≥50 | ≥540 | 111-156 |
100 | ≥195 | ≥390 | ≥26 | - | ≥55 | ≥590 | 111-156 |
The hot rolled plate, long products and fittings as supplied | |||||||
≤20 | ≥235 | 360-460 | ≥27 | - | - | - | - |
20-40 | ≥225 | 360-460 | ≥26 | - | - | - | - |
40-100 | ≥215 | 360-460 | ≥24 | - | - | - | - |
100 | ≥195 | 360-460 | ≥24 | - | - | - | - |
Hot-rolled sheet in the delivery condition. Group strength ОК360В | |||||||
≤2 | ≥235 | 360-530 | - | ≥20 | - | - | - |
2-3.9 | ≥235 | 360-530 | - | ≥22 | - | - | - |
Cold-rolled sheet in the delivery condition. Group strength ОК360В | |||||||
≤2 | ≥235 | 360-530 | - | ≥22 | - | - | - |
2-3.9 | ≥235 | 360-530 | - | ≥24 | - | - | - |
Sheets with a thickness of 12 mm delivery condition (transverse specimens) | |||||||
- | ≥205 | ≥385 | ≥37 | - | ≥60 | - | - |
- | ≥190 | ≥370 | ≥27 | - | ≥59 | - | - |
- | ≥175 | ≥430 | ≥21 | - | ≥51 | - | - |
- | ≥160 | ≥450 | ≥23 | - | ≥49 | - | - |
- | ≥150 | ≥395 | ≥35 | - | ≥62 | - | - |
Description mechanical marks
Name | Description |
---|---|
Section | Section |
sT|s0,2 | Yield strength or limit of proportionality with a tolerance for residual deformation of 0.2% |
σB | Limit short-term strength |
d5 | Elongation after rupture |
d4 | Elongation after rupture |
y | The relative narrowing |
kJ/m2 | Toughness |
Physical characteristics
Temperature | Е, ГПа |
---|---|
20 | 213 |
100 | 208 |
200 | 202 |
300 | 195 |
400 | 187 |
500 | 176 |
600 | 167 |
700 | 153 |
A description of the physical symbols
Name | Description |
---|---|
Е | The normal elasticity modulus |
r | Density |
l | Coefficient of thermal conductivity |
R | UD. the resistivity |
a | The coefficient of linear expansion |
Technological properties
Name | The value |
---|---|
Weldability | Welded without restriction; welding methods: SMAW, ADS submerged arc and gas protection electroslag welding, the CCC. For thickness of more than 36 mm recommended heating and subsequent heat treatment. |
Propensity to temper brittleness | tend not |
Forging temperature | Beginning - 1300 °C, the end - 750 °C. air Cooling. |
Flock-sensitive sensitivity | not sensitive |
Workability by cutting | In the hot rolled condition when blower SB 124 and HB=400 MPa Kn TV.SPL.=1.8 Kn b.St.=1.6 |