Steel R12MF5-MP (ДИ70-MP)
Designation
Name |
The value |
Designation GOST Cyrillic |
Р12МФ5-МП |
Designation GOST Latin |
P12MF5-MP |
Transliteration |
R12MF5-MP |
The chemical elements |
- |
Name |
The value |
Designation GOST Cyrillic |
ДИ70-МП |
Designation GOST Latin |
DI70-MP |
Transliteration |
DI70-MP |
The chemical elements |
CuИ70-MoP |
Description
Steel R12MF5-MP used: for the production of hot rolled and forged strips, hot rolled, forged and calibrated rods, rods with special surface finish produced by hot gas-static pressing (GGP) pulverized powder with subsequent deformation of the blanks; shaped cutters for machining medium alloy steel; taps, broaches, milling cutters for finishing medium alloy, alloyed, corrosion resistant and high strength steels.
Standards
Name |
Code |
Standards |
Sectional and shaped rolling |
В22 |
GOST 1133-71, GOST 2590-2006, GOST 2591-2006 |
Sheets and stripes |
В33 |
GOST 4405-75 |
Sectional and shaped rolling |
В32 |
GOST 7417-75, GOST 28393-89 |
Chemical composition
Standard |
C |
S |
P |
Mn |
Cr |
Si |
Ni |
Fe |
Cu |
N |
V |
Mo |
W |
O |
Co |
GOST 28393-89 |
1.45-1.55 |
≤0.03 |
≤0.03 |
≤0.5 |
3.8-4.3 |
≤0.6 |
≤0.4 |
The rest |
≤0.25 |
0.02-0.06 |
4-4.6 |
1-1.5 |
11.5-12.5 |
≤0.02 |
≤0.5 |
Fe is the basis.
Technological properties
Name |
The value |
Grindability |
1,00-1,20 relative to steel of grade R6M5. |
Resistance to wear |
tool life of 1.50-2.00 in comparison with steel R12MF5. The limit of Flexural strength 3000-4000 MPa. |